Paper · 43rd EU PVSEC · Rotterdam, 2026

Four ways to recover UVID‑affected TOPCon modules, and what happens next in the dark.

UV light damages some new solar modules, but sunlight partly heals them again. In the dark they lose power once more. This study compares four ways to heal a module before testing, and measures how fast it fades afterwards.UV-induced degradation (UVID) in TOPCon modules is metastable: Pmp falls during dark storage and recovers under light containing UVA. The study compares indoor light soaking, outdoor light soaking, consecutive flashing and 365 nm UVA light soaking, then tracks post-recovery dark storage degradation with EL time-lapse imaging.

TitleComparative study of four recovery methods and subsequent dark storage metastability in UV-induced degradation (UVID) affected TOPCon PV modules

A. Nairi, J. Wong, Y. S. Khoo, K. G. Bedrich, F. Lim, S. Nalluri, J. D. Arcebal, T. Reindl, A. G. AberleSERIS, National University of Singapore · Quantified Energy · Sembcorp

Night · EL of one UVID modulePmp 553 W
  • Dark storage
  • Light recovery
Schematic drawn by Quantified Energy.

In brief

  • A UVID-affected module gives a different power reading depending on how long it sat in the dark. That makes fair lab testing hard.
  • Shining UVA light (365 nm LEDs) on the module for 5 minutes healed it as well as indoor light soaking, the reference, with no waiting for it to cool.
  • Repeated flashes from the I-⁠V tester never fully healed it, so flashing should not be used for this.
  • After healing, modules lost about 1% in the first hour and 2.5% in six hours of darkness, with every method tested.

Summary Measuring a field-representative Pmp of UVID-affected TOPCon modules is difficult because Pmp decreases during dark storage and recovers with light exposure. The draft IEC TS 63624-⁠1 prescribes indoor light soaking (1000 Wh/m²) followed by I-⁠V measurement within 4 hours. The study compares four recovery methods, with indoor light soaking at 100 Wh/m² (6 min) as the reference, on dose, time, cooling, handling, energy use and recovery potential. UVA light soaking (365 nm, about 0.5 Wh/m², 5 min) matched light soaking and allowed immediate characterization. Consecutive flashing reached an equilibrium about 2% below UVA recovery (1.3% in the final STC readings). Post-recovery dark storage degradation, tracked by flashing and by EL time-lapse Pmp estimation, was similar for all methods: about 1% after 1 h and 2.5% after 6 h by flash measurement.

Why

A module whose power depends on when you last switched off the lights.

Why · The defect

Deep UV wears down the cell surface.

TOPCon became the dominant solar cell in under three years. Its surface passivation can be damaged by deep UV light below 340 nm, which costs voltage first and current second. In EL images, damaged cells form a checkerboard.

UVID degrades cell passivation and is driven by UV below about 340 nm[2]. It is distinct from LID, LeTID and encapsulant yellowing. Voc drops first, then Isc. Exposure to light containing UVA partially recovers it[3][4].

I-⁠V curve near Pmp · illustrativeUVID

Recovery raises Pmp mainly through voltage. Curve shapes are schematic.

Why · The tropics

More UV, faster UVID.

Sunlight in Singapore carries more UV, and more of the harmful deep UV, than the standard test spectrum. UVID appears there within a year.

Tropical sites receive a higher overall UV dose (≤ 400 nm) and a larger UV-B share. In Singapore UVID appears within about a year, equivalent to a UV dose of about 100 Wh/m².

UV in the spectrum · Singapore vs AM1.5300 to 1200 nm

Values from the study. Singapore, Indonesia, Chile and India are among the higher-risk regions.

Why · The problem

Power falls in the dark and returns in the sun.

In the field, a module recovers every day and fades every night. On its way to the lab it spends a long time in a box. What the lab measures is not what the module delivers on site.

UVID-affected modules are metastable: Pmp decreases during dark storage and recovers under light[3][4]. Packing, transport and unpacking add a long dark period. The draft IEC TS 63624-⁠1 prescribes recovery by indoor light soaking (1000 Wh/m²) and requires I-⁠V measurement within 4 hours.

Pmp at STC over time · schematicDay

Why · In the lab

Four hours may be too long.

One module rated 630 W arrived at 553 W. Light soaking healed it but left it too hot to measure. After an hour of cooling it gave 593 W. Three hours later it had already slipped to 583 W.

Light soaking heats the module, and natural cooling to 25 °C takes about an hour (about 20 min with active cooling). Meanwhile the module degrades in the dark. The 4-hour window is too loose to capture a field-representative Pmp; a recovery method that allows immediate I-⁠V measurement is needed.

One module, nameplate 630 W · standard recovery553 W · −12.2%

Measured values from the study; percentages against nameplate.

How

Four ways to bring a module back before it is measured.

How · Methods

Sun, lamp, flash or UVA LED.

A good method heals at least as well as indoor light soaking, lets the module be measured straight away, and is quick and cheap.

Criteria: recovery at least equal to indoor light soaking (the reference, 100 Wh/m² in 6 min), immediate characterization without cooling or handling, cost and time efficiency.

Facts from the study's comparison table. Schematics drawn by Quantified Energy.

How · Results

UVA LEDs heal as well as the sun, in five minutes.

Each module was measured straight out of dark storage and again after recovery. UVA light matched the best reading and gave the largest gain, with no cooling at all.

Pmp before and after recovery. Outdoor and indoor light soaking included 45 min cooling. Flashing and UVA soaking needed none. On the same module, UVA soaking reached 1.3% more than 120 consecutive flashes.

Pmp before and after recovery · WMeasured

How · Flashing

Flashing stalls short of full recovery.

Each flash heals the module a little, but it fades again between flashes. The two soon balance out, about 2% below what UVA light achieves (1.3% in the final readings).

Under consecutive flashing, Pmp stabilizes at an equilibrium about 2% below the UVA maximum recovery potential (1.3% in the final STC readings). The likely cause is competition between recovery during each flash and dark degradation between flashes.

Pmp through consecutive flashing · schematic of the measured trendFlash 0

Each flash is 100 ms; 120 flashes deliver about 3 Wh/m² over 1 h 30 min.

After

The clock starts the moment recovery ends.

After · Dark storage

EL images watch the module fade.

Flashing the module to check it would also heal it. So a camera took an EL image every 10 minutes for 6 hours, and Quantified Energy's software turned each image into a power estimate.

Flash measurements at 0, 6 and 21 h showed similar dark storage degradation (DSD) for all methods at 6 h, with a slight difference between modules at 21 h. To resolve the first 6 hours without flash interference, EL images were taken every 10 min and Pmp was estimated with Quantified Energy's degradation-mode EL analysis[5]. DSD starts immediately: about 1% after 1 h (EL) and 2.5% after 6 h (flash).

EL time-lapse · 1 image every 10 min0 h · 100%

The fade looks the same whichever method healed the module.

Curves are schematic; the 1% value and the 10-minute cadence are from the study. A slight module-to-module difference appeared after 21 h.

After · Verdict

Recommended: UVA light soaking.

It can be done where the module is measured, it does not heat the module, and it gave the highest power on average.

UVA light soaking ranked first, outdoor light soaking third and the indoor reference second. Consecutive flashing was disqualified for its partial recovery. An alternative is a steady-state sun simulator that recovers the module and measures I-⁠V at STC in one step.

  1. 1UVA light soaking

    5 min · no cooling · no handling · on par with reference

  2. 2Indoor light soaking

    6 min + 1 h cooling · high energy use · reference

  3. 3Outdoor light soaking

    Weather dependent + 1 h cooling · heavy handling

  4. ✕Consecutive flashing

    1 h 30 min · partial recovery only · disqualified

Our part

Quantified Energy's contribution.

Dr Johnson Wong, Dr Yong Sheng Khoo and Dr Karl Bedrich of Quantified Energy co-authored the study with SERIS and Sembcorp. Quantified Energy's quantitative EL analysis made it possible to follow power in the dark without flashing the module.

  • 10 min

    between EL images over 6 hours, each converted to a Pmp estimate[5]

  • 0

    flashes needed to follow dark storage degradation, so flash recovery does not interfere with the result

  • ≈1%

    Pmp lost in the first hour of darkness, resolved in 10-minute steps by EL

  • Field

    The same metastability matters for nighttime drone EL, which images modules hours after sunset. How we report UVID power loss in operation

From lab to field: Quantified Energy images whole plants by night with drone EL.

References

  1. [1]A. Nairi, J. Wong, Y. S. Khoo, K. G. Bedrich, F. Lim, S. Nalluri, J. D. Arcebal, T. Reindl, A. G. Aberle, "Comparative study of four recovery methods and subsequent dark storage metastability in UV-induced degradation (UVID) affected TOPCon PV modules," 43rd European Photovoltaic Solar Energy Conference and Exhibition (EU PVSEC), Rotterdam, 2026, paper 3BO.15.1. EU PVSEC proceedings
  2. [2]A. Sinha, J. Qian, S. L. Moffitt, K. Hurst, K. Terwilliger, D. C. Miller, L. T. Schelhas, P. Hacke, "UV-induced degradation of high-efficiency silicon PV modules with different cell architectures," Progress in Photovoltaics, vol. 31, no. 1, pp. 36–51, 2023. doi:10.1002/pip.3606
  3. [3]T. Karin, "UVID initiates metastability in the dark: how to properly measure unstable Si modules," PV Reliability Workshop, Denver, 2025.
  4. [4]P. Gebhardt, E. Fokuhl, S. S. Mujumdar, H. Frey, A. Beinert, A. Stöhr, M. Kaiser, I. Hädrich, "Stabilization procedures for TOPCon PV modules after UV-induced degradation," Solar Energy Materials and Solar Cells, vol. 294, 113885, 2026. doi:10.1016/j.solmat.2025.113885
  5. [5]"Quantitative electroluminescence image analysis for PV modules: a degradation-mode approach," Quantified Energy, submitted to IEEE Journal of Photovoltaics, under review. Read our summary

This page summarizes the study in plain language. Figures are new schematics by Quantified Energy, not reproductions of the conference figures. The presentation is free to download from the EU PVSEC proceedings.

Make every PV module count throughout its lifetime.

Quantified Energy Labs Pte. Ltd. · 77 Ayer Rajah Crescent, #03-34, Singapore 139954

Presented September 2026