Paper · Under review · IEEE Journal of Photovoltaics

One EL image. Every cell's circuit. The module's power.

A night drone survey has time for one EL picture per module. From how bright each cell glows in that picture, the method works out how damaged each cell is, and from that, how much power the module makes.An EL method anchored to I-⁠V measurements: cell-to-cell variation is constrained to one calibrated degradation mode, so per-cell severity, and a full equivalent circuit, follow in closed form from a single EL image at a fixed drive current.

TitleQuantitative electroluminescence image analysis for PV modules: a degradation-mode approach

J. Wong, K. Bedrich, Y. S. Khoo, J. Chai, F. Lim, A. Nairi, Y. WangQuantified Energy · Sembcorp Solar · SERIS, NUS

EL image · what the drone seesOne module, three steps
  • 1 EL image
  • Severity per cell
  • Voc and Pmax
Schematic drawn by Quantified Energy.

In brief

  • One EL image per module is enough to estimate its open-circuit voltage and maximum power, with a typical error of about 1%.
  • The trick: in a plant, most cells age the same way. We learn that way once, on a few modules, and then only measure how far along it each cell is.
  • Every cell gets its own electrical model, so the module can be re-simulated for any sunlight, temperature or shading.
  • Tested on twenty TOPCon modules with UV-induced degradation (UVID) from a plant in Singapore.

Summary Each cell is described by a lumped equivalent circuit. Instead of fitting every cell freely, all cells are placed on one calibrated line in parameter space, the degradation mode. A single EL image at a fixed drive current then fixes one severity value per cell in closed form, and with it the full circuit. On twenty field-aged TOPCon modules with UVID, each measured after dark storage and after light soaking, predicted Voc and Pmax of the 34 verification module-states reach R² > 0.9 with ≈1% RMSE.

Why

Asset decisions need watts, not defect counts.

Why · The gap

Finding a defect is not the same as knowing its cost.

Most EL software finds, counts and labels defects. Owners, lenders and insurers need to know what those defects do to power. This method links the two.

Computer-vision methods are quantitative at the feature level: counts, areas, classes. Data-driven predictors forecast Pmax or an I-⁠V curve but need large labeled sets and typically cannot be re-evaluated under new conditions without retraining. This work is physics-anchored, calibration-light (≤10 modules) and returns equivalent-circuit parameters per cell.

Three ways to read an EL image · choose oneDefect detection

Schematic comparison based on the literature reviewed in the paper.

Why · The signal

Brightness is voltage.

A cell glows more when its voltage is higher. So an EL image is really a voltage map: each cell's brightness tells us its voltage.

EL intensity follows the local junction voltage exponentially, φ = c · exp(V/Vth). With c shared by all cells of one image, each cell's relative voltage is read directly from its intensity.

From glow to voltage · tap a cellBrightest cell · reference

Every 18 mV less makes a cell about half as bright. Small voltage losses are easy to see.

Physicsφ(r) = c(r) · exp(V(r) / Vth) (1)c is treated as constant across all cells of one image: same optics, glass and angle. Module-to-module variation in c is absorbed by calibration against a reference module. At the 6 A drive current used here, cell voltages span about 85 mV (0.63 to 0.72 V).

How

Learn the way cells age once. Then read each cell along it.

How · The model

Every cell is a small circuit.

Inside each cell, light makes current. Some of it leaks away through defects before it can leave the cell. How much leaks decides the cell's voltage and power.

Each cell is a lumped equivalent circuit: photocurrent JL, n = 1 diode J01, n = 2 diode J02, intrinsic recombination, shunt conductance σsh and series resistance Rs. The cells connect in series to form the module. The output is SPICE-compatible.

Cell equivalent circuit · choose a partLight makes current

Redrawn by Quantified Energy. The reverse-breakdown branch is omitted, as in the paper.

How · The key idea

One dial instead of four.

In a plant, modules are built the same and age the same way. So instead of guessing four numbers per cell, we learn how they change together once. Then each cell only needs one number: how far it has degraded.

Every cell is constrained to a one-dimensional affine subspace, θi = θ0 + si·d, with θ = (JL, J01, J02, σsh). θ0 is the normal cell, d the degradation mode and si ≥ 0 the severity. d is fitted once by MAP calibration, not per module.

Degradation mode · drag the severitys = 0 · normal cell

For these UVID modules, damage mostly raises one kind of leak (J01) and slightly lowers the current from blue light. Together these point to damage near the front of the cell.

Calibrated valuesθ0 = (43.7 mA/cm², 7.404 fA/cm², 1.271 nA/cm², 0) d = (−0.070 mA/cm², 9.997 fA/cm², 0.262 nA/cm², 0)Rs = 0.759 Ω·cm². The mode is J01-dominated: UVID adds recombination in the quasi-neutral regions rather than in the space-charge region or as a shunt, consistent with hydrogen redistribution in the SiNx/poly-Si stack[2]. dJL/dJ01 ≈ −7×10⁹ fits a blue-response loss. Together this points to emitter-side degradation.

How · Inference

From picture to power in four steps.

Once the dial is learned, reading a new module is quick arithmetic. No fitting, no second image, no I-⁠V test.

At inference, each cell's Vi comes from (1) and Jop from the drive current. Substituting the mode into the dark current balance makes it linear in si, which solves in closed form.

Inference · one moduleStep 1 of 4

Module, cell values and curve are illustrative.

Closed formsi = (Jop − J010eVi/Vth − J020eVi/2Vth − Jintr0(Vi) − σsh0Vi) / (dJ01eVi/Vth + dJ02eVi/2Vth + dσshVi) (4)The cell parameters then follow from θi = θ0 + sid, and the module I-⁠V curve is simulated for any condition.

How · Calibration

Calibrate on a few. Apply to the fleet.

Once per module type, a few modules get full lab tests. The model adjusts itself until it matches them. After that, every other module in the plant needs only one EL image.

Calibration is a MAP fit to Voc, Isc, Pmax and EL-derived voltages, starting from published TOPCon values with a small L2 prior. An inner loop fixes c through a reference cell and matches the simulated Isc distribution. RMS error falls by more than an order of magnitude in about eight iterations.

Calibrate once · then one image per moduleCalibrating

Needed for calibration: at least three modules (five to ten recommended), at least two EL images and a 1-Sun I-⁠V test for each.

Error curve shape is illustrative; the drop of more than 10× within about eight iterations is as reported. Calibration needs ≥3 modules (5 to 10 recommended) spanning the field EL range, ≥2 EL images each including one at Iref, and a 1-Sun I-⁠V per module.

Proof

Twenty field modules, two states, one image each.

Proof · The test

Thirty-four blind tests.

Twenty TOPCon modules came from a plant in Singapore. Each was measured twice: after about two months in the dark, when UV damage shows most, and after light soaking, when it partly recovers. Three modules (six measurements) calibrated the method. The other 17 modules (34 measurements) tested it.

Twenty TOPCon modules fielded for at least six months in Singapore were measured at STC after extended dark storage and after 1 h light soaking at 1000 W/m², with EL at 6 A (≈40% Isc) and 1 A. Modules 1, 17 and 19 (lowest, mid and highest mean EL) calibrated the model; the remaining 34 module-states verified it.

20 modules · EL at 6 A · schematicAfter dark storage

Tiles are drawn by Quantified Energy to show the pattern, not copies of the measured images.

Proof · Accuracy

About 1% error on power, from one image.

For the 34 test measurements, the predicted voltage and power matched the lab results closely. Calibrating on all twenty modules instead of three barely changed that.

On the 34 verification module-states, from one 6 A EL image each. Recalibrating on all 40 module-states leaves the mode essentially unchanged (dJ01 within 0.02%, dJL within 2%) and mainly improves FF.

R² against lab I-⁠V · RMSE in brackets3 calibration modules
0.93

R² for open-circuit voltage, 0.6% RMSE

0.91

R² for maximum power, 1.1% RMSE

3

modules were enough to calibrate

Short-circuit current is harder to predict from EL, as it also depends on optical differences from manufacturing.

Outliers. Modules 7, 15 and 16 in the dark-stored state show simulated Voc about 1 V high (≈14 mV per cell), suspected to be partial UVID recovery between the I-⁠V flash and EL acquisition 20 to 25 h later. The offset persists with all-module calibration, so it comes from the measurement sequence, not the calibration. Isc R² is a moderate 0.632, as Isc also depends on optical variation the mode does not capture. Temperature effects are an order of magnitude smaller (<1 mV for a 2 K module-to-module difference).

Proof · What it reveals

Watch UV damage recover in the light.

After dark storage, many cells are badly degraded and the spread is wide. After light soaking, most cells recover and bunch together. The method sees this from the images alone.

Inferred severity shifts from a broad, right-skewed dark-storage distribution to a narrow peak after light soaking, consistent with largely reversible, metastable UVID.

Cell severity, all 20 modules · schematic distributionAfter dark storage

Shapes are schematic, following the paper's description.

Proof · One image or two

One image is enough for power. Two can flag the odd cell out.

Using two EL images per module gave no better power predictions. But comparing each cell with the expected pattern may expose cells that look normal in EL and are not.

Free two-image fits of (J01, J02) at 1 A and 6 A stay within about 2 nA/cm² of the mode in J02 and give no gain in aggregate Voc, Isc or Pmax. Their likely value is the residual, which may map anomalies such as high-J02 or shunted cells. This was not yet investigated systematically.

Module 14, after light soaking · schematicEL image at 6 A

Cell positions follow the paper's description of module 14; drawing by Quantified Energy.

Use

Built for drones flying a whole plant at night.

Use · In the field

Designed around one image per module.

At night, the modules are driven with current so they glow, and the drone flies over them. There is time for one image per module. This method turns that one image into power.

6 A (≈40% Isc) is the operating point of QE's drone-coupled EL system, balancing signal-to-noise against current-ramp time and cell heating. It sits well inside the c·exp(V/Vth) regime. The framework is current-agnostic; the IEC TS 60904-⁠13 100% / 10% Isc convention can be used in the lab.

From the Quantified Energy motion library.
  • Power per module

    Voc and Pmax for every module imaged, not a sample.

  • A circuit per cell

    Re-simulate under any irradiance, temperature, shading or string layout.

  • Mechanism clues

    In this study, the pattern of change helped tell UVID apart from potential-induced degradation (PID).

    J01-dominated, current-independent contrast points to UVID rather than PID-p or PID-s.

  • Anomaly map

    With a second EL image at another current, cells far from the common pattern, such as cracks or bypass faults, stand out for follow-up.

Use · In QE's analysis

From image to power at plant scale.

In QE's EL analysis, the step that models each cell and predicts the module I-⁠V curve is where a per-cell circuit like this one fits.

From the Quantified Energy motion library.

More on UVID: measuring real-world power loss of UVID-affected TOPCon modules, and UVID recovery and dark-storage metastability, where this method tracked module power from EL every 10 minutes.

Use · Limits

What the study does not yet show.

All twenty modules came from one production batch with one type of damage. Other module types and other kinds of damage still need to be tested.

The validation set is twenty modules from a single production batch, all with the same UVID mode. Results should not be assumed to generalize to other module types, manufacturers or mechanisms without further validation. Localized failures (broken interconnects, shorted bypass diodes, severe cracks) are outside a single global mode and are handled as residual anomalies. Data will be deposited in a public repository upon publication.

Our part

Quantified Energy's contribution.

Five of the seven authors are from Quantified Energy, with co-authors from Sembcorp Solar and SERIS, National University of Singapore.

  • 5 of 7

    authors from Quantified Energy: J. Wong, K. Bedrich, Y. S. Khoo, J. Chai, Y. Wang

  • 1 image

    per module at inference, matching what a night drone survey can capture

  • ≈1%

    RMSE on maximum power across 34 verification module-states

  • 2018 → 2026

    four of the authors co-wrote a 2018 IEEE JPV paper on quantitative EL for PID-affected modules[3]

References

  1. [1]J. Wong, K. Bedrich, Y. S. Khoo, J. Chai, F. Lim, A. Nairi, Y. Wang, "Quantitative electroluminescence image analysis for PV modules: a degradation-mode approach," IEEE Journal of Photovoltaics, manuscript under review.
  2. [2]M. U. Khan et al., "UV-induced degradation in TOPCon solar cells: hydrogen dynamics and impact of UV wavelength," Solar Energy Materials and Solar Cells, vol. 294, 113895, 2026.
  3. [3]K. G. Bedrich et al., "Quantitative electroluminescence imaging analysis for performance estimation of PID-influenced PV modules," IEEE Journal of Photovoltaics, vol. 8, no. 5, pp. 1281–1288, 2018.

This page summarizes a manuscript that is under review at IEEE Journal of Photovoltaics. The text is a plain-language summary and all figures are new schematics drawn by Quantified Energy, not reproductions of the manuscript figures. Figures marked schematic are illustrative; numbers are as reported in the manuscript.

Make every PV module count throughout its lifetime.

Quantified Energy Labs Pte. Ltd. · 77 Ayer Rajah Crescent, #03-34, Singapore 139954

Under review · November 2026